Metallic oxide layer of heat resistant element contributes to the high-temperature oxidation resistance by delaying the oxidation,
and also has positive effect on the electrical resistivity increase. In this study, the green compacts of Fe-Cr-Al powder mixed
with STS434L were oxidized at 950°C up to 210 hrs in order to consider the effect of metal oxide on the oxidation and electrical
resistance. It exhibited the low oxidation resistance in case of 434L only, however it increased as the amount of Fe-Cr-Al powder
in the 434L compact. The higher electrical resistivity was observed at the Fe-Cr-Al compact with and 434L powder. The metal
oxides of (Fe0.6C0.4)2O3, Cr2O3, and Fe2O3 contributed to the electrical resistivity, whereas Al2O2 took a role of oxidation resistance.
Ta witryna wykorzystuje pliki cookies do przechowywania informacji na Twoim komputerze. Pliki cookies stosujemy w celu świadczenia usług na najwyższym poziomie, w tym w sposób dostosowany do indywidualnych potrzeb. Korzystanie z witryny bez zmiany ustawień dotyczących cookies oznacza, że będą one zamieszczane w Twoim komputerze. W każdym momencie możesz dokonać zmiany ustawień dotyczących cookies
Informacja
SZANOWNI CZYTELNICY!
UPRZEJMIE INFORMUJEMY, ŻE BIBLIOTEKA FUNKCJONUJE W NASTĘPUJĄCYCH GODZINACH:
Wypożyczalnia i Czytelnia Główna: poniedziałek – piątek od 9.00 do 19.00